Testing acc. to BMW AA-0772 test: Resistance of leather to oleic acid
Material
Industry
Publisher
Testing methods
Our test laboratory performs testing according to BMW AA-0772 to determine the resistance of leather to oleic acid. The method assesses whether exposure to oleic acid followed by mechanical surface loading causes visible damage to the leather finish or surface.
Oleic acid is used as a defined test medium to simulate fatty substances that can come into contact with automotive leather during use. The subsequent mechanical loading makes it possible to identify weakening of the surface caused by the chemical exposure.
Applications
AA-0772 is particularly relevant for automotive leather used on seats, steering-related interior surfaces and other components exposed to frequent human contact.
The method can be used in leather and finish development, material approval and quality assurance to compare different finishing systems, leather qualities and production batches with regard to resistance to fatty media and subsequent mechanical stress.
Testing according to BMW AA-0772
The conditioned leather specimen is placed grain side up on a firm support. A standardized textile is positioned on the leather and impregnated uniformly with oleic acid. A glass plate is placed on top to ensure defined contact.
The specimen is then subjected to elevated-temperature storage. After exposure, the textile and glass plate are removed, excess oleic acid is carefully removed and the leather is reconditioned.
The exposed area is subsequently subjected to repeated mechanical loading in a Crockmeter using a defined test tip. The surface is then visually examined for damage. Particular attention is paid to abrasion, flaking, peeling and rupture of the leather surface; slight marking may be distinguished from unacceptable severe abrasion.
Related tests
The mechanical assessment in AA-0772 is closely related to BMW GS 97034-8 – Determination of marring resistance, which FILK offers as an accredited test method.
The Crockmeter principle is also used in DIN EN ISO 105-X12 – Colour fastness to rubbing.
For evaluating automotive surface materials against fatty or oily media, FILK also offers VDA 230-225 (6) – Exposure to fat or oil.
Further BMW-specific test methods can be found in our overview of testing according to BMW specifications; for access to our complete range of testing services and to search for specific standards, specifications and test methods, visit the FILK accredited test laboratory – testing services and standards search. For material and technology-related problems in automotive interiors, FILK provides failure analysis and defect diagnostics to systematically identify possible causes.